A LiFePO4 pack is normally bought for cycle life: 3,000 to 5,000 cycles is routine, against 300 to 500 for lead-acid. Almost every premature failure we see in the field is not a cell defect. It is a charging profile borrowed from lead-acid, applied to a chemistry whose voltage curve is so flat that nothing looks wrong until capacity is already gone.
Lead-acid 12V charging ends in a float hold around 13.5 V, with absorption near 14.4 V and, on many models, a periodic desulfation pulse that can reach 15 to 16 V. A 4S LiFePO4 pack wants a fixed ceiling of 14.6 V, which is 3.65 V per cell, and no long float at all. Connect the two and one of two things happens. Either the pack sits permanently at 80 to 90 percent state of charge, because absorption ends too early and float is too low to finish the job, or the desulfation pulse drives it past the cell ceiling and the BMS disconnects. Repeated nuisance disconnects are their own wear mechanism, and they hide the real problem: the profile was never matched to the chemistry.
Charge current is usually set between 0.2C and 0.5C. For a 100Ah pack that means 20 to 50 A; for a 280Ah golf cart pack it means 56 to 140 A. Below roughly 0.1C the pack still charges, but the balancing circuit has very little time at the top of the curve to move energy between cells, so an imbalanced pack stays imbalanced. Above 0.5C the heat generated inside the cells starts to cost cycle life, and the gain in charge time is smaller than the arithmetic suggests, because the constant-current stage is only part of the cycle.
The number that actually governs this is the BMS continuous charge rating, not the charger nameplate. A charger able to deliver 50 A into a pack whose BMS permits 30 A does not charge faster. The BMS throttles, or it opens the contactor, and the operator experiences a charger that randomly stops. Specify the charger to the pack: voltage class from the cell count, current from the BMS, and a little headroom above the expected load so the unit is not running at 100 percent of rating in a hot cabinet.
The absorption voltage is simply cell count multiplied by 3.65 V. Four cells in series gives 14.6 V, eight gives 29.2 V, sixteen gives 58.4 V. The charger holds that ceiling while current tapers, and it should terminate when current falls to roughly 0.05C: about 5 A on a 100Ah pack, about 14 A on a 280Ah pack. That taper is where the last 10 to 15 percent of capacity goes in, and it is also where most of the stress accumulates.
Holding 14.6 V for another four hours after the current has already collapsed adds one or two percent of capacity and a disproportionate amount of calendar aging. This is the single most common mistake in RV and marine installations, where the charger is on shore power for weeks and the pack is left parked at its maximum voltage the entire time.
Lead-acid wants to be floated; that is how it stays healthy and ready. LiFePO4 does not. A pack held at 3.65 V per cell is a pack held at 100 percent state of charge, and calendar aging accelerates sharply above about 80 percent, especially at elevated ambient temperature. If the application genuinely requires the charger to stay connected, as in a standby cabinet, a marine house bank or a vehicle that sits for months, float at 3.35 to 3.40 V per cell instead. That is 13.4 to 13.6 V for a 4S pack, and it holds the bank near 95 percent without pressing on the cells.
Do not charge below 0 degrees Celsius. Lithium plating at the anode is not reversible, and a single cold charge can remove a measurable slice of capacity permanently. The BMS should block charging in that window, and a charger with its own NTC probe on the pack is a useful second line of defence, because a BMS that is asleep or misconfigured cannot protect anything.
At the other end, derate above roughly 45 degrees Celsius ambient. A sealed charger inside a cabinet in direct sun can see 15 degrees more than the air outside it, so a unit rated for 40 degrees ambient is not the same product in a Texas parking lot in August. Storage is a separate question again: if a pack will sit idle for months, leave it near 50 percent state of charge, in a dry place, and top it up every few months rather than storing it full.
Voltage class: cell count multiplied by 3.65 V. Charge current: around 0.3C, capped by the BMS continuous rating. Termination: about 0.05C, then stop, do not float at ceiling. Float, if required: 3.35 to 3.40 V per cell. Temperature: no charge below 0 degrees, derate above 45 degrees ambient. Enclosure: IP rating matched to where the unit actually lives, and connectors rated at least as high as the enclosure. Those seven lines remove nearly all of the ambiguity that turns a good pack into a short-lived one.
Related models: a 12V LiFePO4 and lead-acid charger (14.6 V, 10 A) for 4S packs, 14.6 V 50 A where the bank is large, and the 14.6 V 20 A waterproof on-board unit for marine and vehicle-mounted installations.